Студопедия — Test specimens
Студопедия Главная Случайная страница Обратная связь

Разделы: Автомобили Астрономия Биология География Дом и сад Другие языки Другое Информатика История Культура Литература Логика Математика Медицина Металлургия Механика Образование Охрана труда Педагогика Политика Право Психология Религия Риторика Социология Спорт Строительство Технология Туризм Физика Философия Финансы Химия Черчение Экология Экономика Электроника

Test specimens






 

The metal specimens used for the axial tension have either a round or a rectangular section.

The dimensions and production standards of the specimens are given in GOST 1497-84. The specific features of the specimens are strengthened places to be installed in the grips of the testing machine, and the gradual change of sections.

While producing specimen from blank parts, certain precautionary measures are taken to exclude any changes of metal properties caused by heating or hardening.

To determine the degree of change of the gage length after the rupture, certain hachures are marked by a dividing machine on the testing surface in every 10 mm all along the length.

The main dimensions of cylindrical specimens are shown in Fig.6 and their values from GOST 1497-84 are given in the table 1.

 

 


Fig. 6. Types of proportional cylindrical specimens for tensile test

(GOST 1497-84)

 

Specimen number d0 L_=5d0 L_=10d0 d0 D h1 H2 r
               
               
               
               
               
            2, 5 1, 5
            2, 5 1, 5
            2, 5 1, 5
            2, 5 1, 5

 


Order

1. Study the basic theoretical statements and the conditions to conduct the tensile test, testing machine and specimens.

2. Prepare the testing machine for work: switch on the main switch in the power cabinet, switch on the packet-type switch of the loading apparatus and the controlling unit, switch on the button " POWER", fill the diagram registration unit with the ink and insert a diagram form. All this is done by the teaching-foreman.

3. Choose a specimen you need from table 1 (№7).

4. Place the travelling cross-bar so as you can insert a specimen in the grips. For this you have to press the button " START", then press the button " UP" or " DOWN" depending on the required movement direction of the cross-bar. At the right position of the cross-bar press the button " STOP".

5. Insert the specimen into the grips of the loading unit and cramp it.

6. To eliminate the clearances, apply the initial load of 1, 0 kN by pressing the buttons " START", " DOWN", " STOP" in a sequence.

7. Put the zero values on the indicator panel " LOAD" and " DISPLACEMENT" by pressing the buttons " TESTING REGIMES".

8. Conduct the specimen test up to the rupture by pressing the buttons " START" and " DOWN" in sequence. After the rupture of the specimen press the button " STOP". In the process of testing watch the indicator and the diagram registration.

9. Write down the last value on the indicator panel " LOAD" - Fut.

10. Print the diagram " F~Δ L " (Fig.4).

11. Draw the diagram " " (Fig.4) in a corresponding scale.

12.1 By the diagram " " find the basic mechanical characteristics of the material tested.

Determine the modulus of the extension elasticity from the diagram " ". For the linear region of the diagram (Fig.4) we have

(MPa)

12.2. Determine the proportional limit from the diagram " ". From the coordinate basic origin (Fig.6) draw a straight line OM coinciding with the initial region of the tension diagram. Then, on the arbitrary value of the stress draw a straight line AB, being parallel to the axis of abscissa. On this line measure off the kn length which is equal to half of the mk length. Through the n point and the coordinate basic origin draw the On line and then draw the CD tangent parallel to it to the diagram. The tangent point determines the target value .

 

Fig.6. Graphical way to determine the proportionality limit.

 

12.3. Determine the elastic limit . On the ‘ ’ axis measure off the residual deformation = 0, 0005, then through this point draw a straight line parallel to the linear region of the diagram (see Fig.7). The crossing point of the straight line and the diagram determines the value .

 

 

Fig.7. Graphical way to determine the elastic limit

 

12.4. Determine the yield point (yield strength ). On the “ ” axis measure off the residual deformation =0, 002, then, through this point draw a straight line parallel to the initial linear region (Fig.8). The crossing point of the straight line and the diagram determines the value ().

Fig.8. Graphical way to determine the yield point

 

12.5. The breaking strength is the maximum value on the " " diagram.

12.6. Determine the nature of the specimen rupture. The typical specimen ruptures of different materials are shown in Fig.9.

 

а) b) c)

 

Fig 9. Types of specimen ruptures in tension:

a - necking rupture (low-carbon steel);

b - rupture by separation (cast iron);

c - rupture by cut-off (aluminum alloys magnesium strained)

 

12.7. Determine the plasticity characteristics.

The relative elongation of the specimen, broken in the middle part of the gage length, is determined by the specimen gage length, marked symmetrically to the middle part before risks testing, and by the total elongation, which is measured after the rupture upon caused risks, as the difference L-L0 (Fig.10). To receive the correlate results in the time of the specimen rupture at the end regions of the gage length, equal sections are drawn in 10 mm, and Δ L is determined supposing that the rupture has taken place in the middle part. The measured length of the gage length has to be calculated from the relation:

 

L=bc+cf, bc=ab+ac

 

where ab is the length of the region from the rupture place of the extreme mark b to the direction of the short mark until the mark c; cf is the length of the region from the mark c to the rupture direction of e mark, constituting as many sections as there are in the region from the mark c to the extreme mark f (to the end B).

The percentage of elongation is determined by the formula

 

 

Fig.10. Determining the percentage of elongation and reduction

 

The reduction in the area of a cylindrical specimen can be determined using the middle value of the diameter in the rupture place, calculated in two mutually perpendicular directions. In the case of testing the plate specimens (GOST 1497-84), as a rule, it is not recommended to determine the value of the reduction in the area. If it is necessary to determine area of the cross-section area АК in the rupture place, it can determined by multiplication of the maximum length of the specimen in the rupture place m and the minimum thickness n.

The percentage reduction in the area after breaking is determined by the formula

 

12.8. Determine the grade of the material by the results of virtual testing from table 2, taken from the handbook of materials.

 

Material Е ()
MPa %
Steel Ct.3              
Steel H18K9MST              
Steel 30XrCH2A              
Cast iron C410           0, 2  
Cast iron B435              
Brass J196              

Report

The report must include:

1. The title page.

2. The goal of the work.

3. The description of equipment and specimens.

4. Tension diagram and its processing.

5. The testing results.

 


6. Test questions answered.

7. Conclusion.

 







Дата добавления: 2014-11-10; просмотров: 1042. Нарушение авторских прав; Мы поможем в написании вашей работы!



Композиция из абстрактных геометрических фигур Данная композиция состоит из линий, штриховки, абстрактных геометрических форм...

Важнейшие способы обработки и анализа рядов динамики Не во всех случаях эмпирические данные рядов динамики позволяют определить тенденцию изменения явления во времени...

ТЕОРЕТИЧЕСКАЯ МЕХАНИКА Статика является частью теоретической механики, изучающей условия, при ко­торых тело находится под действием заданной системы сил...

Теория усилителей. Схема Основная масса современных аналоговых и аналого-цифровых электронных устройств выполняется на специализированных микросхемах...

Деятельность сестер милосердия общин Красного Креста ярко проявилась в период Тритоны – интервалы, в которых содержится три тона. К тритонам относятся увеличенная кварта (ув.4) и уменьшенная квинта (ум.5). Их можно построить на ступенях натурального и гармонического мажора и минора.  ...

Понятие о синдроме нарушения бронхиальной проходимости и его клинические проявления Синдром нарушения бронхиальной проходимости (бронхообструктивный синдром) – это патологическое состояние...

Опухоли яичников в детском и подростковом возрасте Опухоли яичников занимают первое место в структуре опухолей половой системы у девочек и встречаются в возрасте 10 – 16 лет и в период полового созревания...

Тема: Кинематика поступательного и вращательного движения. 1. Твердое тело начинает вращаться вокруг оси Z с угловой скоростью, проекция которой изменяется со временем 1. Твердое тело начинает вращаться вокруг оси Z с угловой скоростью...

Условия приобретения статуса индивидуального предпринимателя. В соответствии с п. 1 ст. 23 ГК РФ гражданин вправе заниматься предпринимательской деятельностью без образования юридического лица с момента государственной регистрации в качестве индивидуального предпринимателя. Каковы же условия такой регистрации и...

Седалищно-прямокишечная ямка Седалищно-прямокишечная (анальная) ямка, fossa ischiorectalis (ischioanalis) – это парное углубление в области промежности, находящееся по бокам от конечного отдела прямой кишки и седалищных бугров, заполненное жировой клетчаткой, сосудами, нервами и...

Studopedia.info - Студопедия - 2014-2024 год . (0.009 сек.) русская версия | украинская версия